React2FireAll articles →
Insight

Discharging lithium-ion batteries for safe recycling: how low should the voltage go?

Spent lithium-ion batteries still hold most of their energy, and opening or shredding a charged cell can trigger thermal runaway. A study in the Journal of Cleaner Production sets a clear end-point for safe dismantling (below 1.5 V) and proposes a faster, corrosion-free way to reach it.

Dr. Fouad Laoutid · Flame retardancy of polymers & composites

A battery retired from an electric vehicle still keeps 70–80% of its initial capacity. During dismantling and shredding, that energy can be released at once: an internal short circuit, a lithiated anode reacting with air moisture, and the cell goes into thermal runaway. This is why recyclers discharge cells before any mechanical step. The open questions are how far to discharge, and how to do it quickly without creating new problems.

Why lithium-ion cells are a fire hazard

A lithium-ion cell combines a large amount of stored energy with a flammable organic electrolyte. If it is overheated, crushed, pierced or short-circuited, a chain of exothermic reactions can start: the protective layer on the anode breaks down, the separator melts and causes an internal short circuit, and layered oxide cathodes can release oxygen. Once this thermal runaway is under way it sustains itself. The cell vents flammable and toxic gases (hydrogen, carbon monoxide, hydrocarbons and hydrogen fluoride), which can burn as jet flames or accumulate and explode. Heat spreads from cell to cell, and a battery that seems extinguished can reignite hours later. Spent batteries hidden in waste streams are already a frequent cause of fires in collection and sorting facilities.

A study by Wu and co-workers at the Chinese Academy of Sciences addresses both questions.[1]

Two ways to discharge, both with drawbacks

How far is far enough?

The authors discharged spent NMC and LFP pouch cells well below their normal operating range, then looked at bulging, sparking on short circuit, gas composition, lithium content of the electrodes and the reactivity of the opened anode with water.

A faster discharge without corrosion

In 0.5 M NaCl, the aluminium tab of the cell was almost completely corroded within two hours, and the discharge slowed down accordingly. The authors made three changes:

Together, the reductant and ultrasound cut the discharge time by at least three quarters. A cell with 6.5 Ah left reached less than 1 V in 55 hours, whereas in a conventional solution less than 3.5 Ah had been released after about 250 hours, at 2 V. LFP cells responded in the same way.

Abuse tests confirm the threshold

Cells discharged below 1.5 V with the new method were short-circuited with a copper wire, pierced with a 2 mm steel nail and crushed. There was no spark, no smoke and no noticeable temperature rise, and the separator was not deformed after crushing. The short-circuit and nail tests were repeated on five cells each, with the same result.

What it means in practice

References

  1. Wu L., Zhang F.-S., He K., Zhang Z.-Y., Zhang C.-C. Avoiding thermal runaway during spent lithium-ion battery recycling: a comprehensive assessment and a new approach for battery discharge. J. Clean. Prod. 380 (2022) 135045. doi:10.1016/j.jclepro.2022.135045
  2. Regulation (EU) 2023/1542 of the European Parliament and of the Council of 12 July 2023 concerning batteries and waste batteries. Official Journal of the European Union L 191 (2023) 1–117.
Share on LinkedInDiscover React2Fire